Material Notes:
Supreme Steel 410 provides good corrosion resistance plus high strength and hardness. It is magnetic in both annealed and hardened conditions. A wide range of properties can be developed with different heat treatments. Applications requiring moderate corrosion resistance and high mechanical properties are ideal for this alloy. Typical uses include flat springs, knives, kitchen utensils and hand tools.
Applications: Bearings Bushings Cutlery Dies Fasteners Hand tools Plastic molds Pump shafts Screens Steam/Gas Surgical instruments Turbine blades Valves/Valve components
Corrosion Resistance: corrosion resistance and high mechanical properties.
UNS S41000, ASTM A182, ASTM A276, ASTM A479
Chemical Composition Limits | |||||||
Weight% | C | Si | Mn | P | S | Cr | Fe |
Alloy 410 | 0.15 max | 1.0 max | 1.0 max | 0.040 max | 0.030 max | 11.5-13.5 | Bal |
Typical Mechanical Properties | |||||||
Material | Tempering Temp °C (°F) |
0.2 % Yield Strength (Mpa) | Ultimate Tensile Strength (Mpa) | % Elongation in 2" | % Reduction of Area | Charpy V Notch Impact Strength (J) | Hardness Brinell |
Alloy 410 Bar Hardened 1850°F (1010°C) 30 mins, oil quench, tempered 4 Hrs |
260 (500) | 1089 | 1331 | 17 | 62 | 76 | 401 |
Alloy 410 Bar Hardened 1850°F (1010°C) 30 mins, oil quench, tempered 4 Hrs |
317 (700) | 1069 | 1296 | 17 | 60 | 66 | 401 |
Alloy 410 Bar Hardened 1850°F (1010°C) 30 mins, oil quench, tempered 4 Hrs |
482 (900) | 1014 | 1303 | 18 | 58 | 38 | 401 |
Alloy 410 Bar Hardened 1850°F (1010°C) 30 mins, oil quench, tempered 4 Hrs |
538 (1000) | 917 | 965 | 19 | 62 | 33 | 285 |
Alloy 410 Bar Hardened 1850°F (1010°C) 30 mins, oil quench, tempered 4 Hrs |
593 (1100) | 724 | 827 | 20 | 63 | 52 | 248 |
Alloy 410 Bar Hardened 1850°F (1010°C) 30 mins, oil quench, tempered 4 Hrs |
649 (1200) | 634 | 731 | 21 | 65 | 119 | 223 |